Ni-Zn MATERIALS FOR INDUCTANCE |
|
| Characteristics |
Initial Permeability |
Frequency
Range |
Relative
Temp-coeft |
Reiltive
Loss Factor |
Saturation
Flux Density |
Curie Temp |
Electrical
Resistivity |
Density |
| Symbot |
ui |
f |
ui |
tan/ui |
Bs |
Tc |
P |
d |
| Unit |
( 25%) |
MHz |
10-6/ (20~60 ) |
10-6/ (MHz) |
mT(Oe) |
 |
-m |
g/cm3 |
| JPL9H |
900 |
0.05~1 |
15~35 |
< 150(1) |
350(20) |
120 |
106 |
5 |
| JPL6H |
600 |
0.1~1.5 |
15~35 |
<70(1.5) |
350(20) |
150 |
106 |
4.9 |
| JPL4H |
400 |
0.1~2 |
10~20 |
<500(2) |
240(20) |
130 |
106 |
4.6 |
| JPL3H |
300 |
0.1~2 |
15~35 |
<105(2) |
350(20) |
200 |
106 |
4.8 |
| JPL2H |
200 |
0.3~7 |
15~35 |
<105(7) |
360(20) |
200 |
106 |
4.8 |
| JPL60 |
60 |
0.5~15 |
5~15 |
< 250(15) |
300(50) |
300 |
106 |
4.8 |
| |
Ni-Zn MATERIALS FOR EMI-SUPPRESSOR |
|
| Characteristics |
Initial Permeability |
Frequency
Range |
Relative
Temp-coeft |
Curie Temp |
Electrical
Resistivity |
Density |
| Symbot |
ui |
f |
ui |
Tc |
P |
d |
| Unit |
( 25%) |
MHz |
10-6/ (20-60 ) |
 |
-m |
g/cm3 |
| JPZ-1.5K |
1500 |
1~500 |
0-3 |
110 |
106 |
5 |
| JPZ-1K |
1000 |
1~500 |
2-5 |
120 |
106 |
5 |
| JPZ-5H |
500 |
1~500 |
8-15 |
130 |
106 |
4.8 |
| JPZ-4H |
400 |
1~500 |
10-20 |
130 |
106 |
4.6 |
|
|